In dissolving metals or especially mixtures thereof by strong acids, there is always a risk of precipitation
(e.g.: Pb and Ba with sulfuric acid, Ag with hydrochloric acid, Al may form oxides/oxide-hydrates and the
like). Even if these elements often are not covered by legislation, there is the risk of loss of target analyte
due to co-precipitation. For this standard it has to be assured that no target elements are lost in the test
sample solution. So any remnants have to be checked either by different methods, whether they contain
target elements or the remnants after acid dissolution are to be dissolved completely by further dissolution
methods (such as alkali fusion or use of an airtight pressurized vessel). The so treated, formerly remnants
are then combined with acid-dissolved solution for measurement.
Common methods for sample digestion
A glass beaker containing the sample is covered with a watch glass. 20 ml of mixed acid 1 is added and
the beaker is heated until the sample has been dissolved. After cooling to room temperature, the
underside of the watch glass and inside wall of the beaker are rinsed with water, and the watch glass is
removed. The solution is transferred to a 100 ml volumetric flask and the flask then filled with water to 100
ml. The resulting solution is the concentrate sample solution. The concentrate sample solution is diluted
with water to the appropriate concentration level for each measurement apparatus. If necessary, an
internal standard element, rhodium, for example, is added before the flask is filled with water. The type of
element and its amount depend on the analytical method selected. The particular paths of dilution have to
be taken into account in the calculation of results. Both, dilution and internal standard addition have to be
documented in the test report.
If containing zirconium, hafnium, titanium, tantalum, niobium or tungsten
A PTFE/PFA beaker containing the sample is covered with a watch glass. 20 ml of mixed acid 2 is added
and the beaker is heated until the sample is dissolved. After cooling to room temperature, the underside of
the watch glass and inside wall of the beaker are rinsed with water, and the watch glass is removed. The
solution is transferred to a 100 ml volumetric flask and the flask is filled with water to 100 ml. The resulting
solution is the concentrate sample solution. The concentrate sample solution is diluted with water to the
appropriate concentration level for each measurement apparatus. If necessary, an internal standard
element, rhodium, for example, is added before the flask is filled with water. Because of the use of
hydrofluoric acid, the internal standard should not comprise rare earth elements. The type of element and
its amount depend on the analytical method selected. The particular paths of dilution have to be taken into
account in the calculation of results. Both, dilution and internal standard addition have to be documented
in the test report.
If containing tin
A beaker containing the sample is covered with a watch glass. 10 ml of mixed acid 3 is added in small
quantities. After violent reaction ends, the beaker is heated slowly until the sample is dissolved
completely. After cooling, the underside of the watch glass and inside wall of the beaker are rinsed with
water, and the watch glass is removed. 10 ml of sulfuric acid is added and the beaker is heated until white
fumes of SO3 are liberated. After cooling for several minutes, 20 ml of hydrobromic acid are added, and
the beaker is heated until white fumes are visible. This process is repeated three times. After cooling to
room temperature, 10 ml of nitric acid is added to dissolve salts. After cooling to room temperature, the
solution is transferred to a 100 ml volumetric flask which is then filled with water to 100 ml. The resulting
solution is the concentrate sample solution. The concentrate sample solution is diluted with water to the
appropriate concentration level for each measurement apparatus. If necessary, an internal standard
element, rhodium, for example, is added to the flask before filling with water. The type of element and its
amount depend on the analytical method selected. The particular paths of dilution have to be taken into
account in the calculation of results. Both, dilution and internal standard addition have to be documented
in the test report.
15.6.3 Preparation of laboratory reagent blank
Procedure identical to preparation of test sample solution is executed concurrently without sample.
15.7 Test Procedure
The calibration curve method is used for sample measurement. If the sample composition can be
identified clearly, the calibration method (matrix matching method) is used. If it is unknown, the internal
Version 1.0
12/6/2004
64 of 79