determined through the use of an Instron machine. The static samples were compared to the
conditioned samples to determine the effectiveness of our device.
5.5.2 Experimental Results
Two individual trials were conducted, each consisting of two time points (3 and 7 day), in which both
static (control) and mechanically conditioned (experimental) samples were examined for UTS, thickness,
and cell density.
For the first trial (Figure 35) the average UTS of unconditioned samples after a three day culture period
was 555.92 ± 129.78 kPa, whereas conditioned samples after 3 days were found to have a mean UTS of
429.60 ± 107.33 kPa (p = 0.19, therefore not statistically different). For the 7 day samples,
unconditioned rings were found to have a UTS of 82.79 ± 13.29 kPa while the conditioned rings were
measured to have a UTS of 122.42 ± 32.96 kPa (p = 0.052, therefore not statistically significant). The
UTS for both static and conditioned ring samples were significantly stronger at 3 days compared to 7
days (p<0.001).
Figure 35. Ultimate tensile strength first trial. N-values are 2, 3, 2, and 4, respectively.
These calculations were repeated for the second trial (Figure 35). After three days of culture, the static
samples exhibited an average UTS of 128.23 ± 36.8 kPa, whereas the conditioned samples were found
be able to withstand 160.27 ± 31 kPa before failing (p = 0.18, therefore not statistically different). After
seven days of culture, the static samples experienced a UTS of 84.19 ± 19.4 kPa compared to the